China Glass Factory · Technical answers

What is heat soak testing (HST) and when is it required for tempered glass?

Heat soak testing re-heats tempered glass to about 290 °C for two hours so that any pane containing nickel sulphide inclusions breaks in the oven instead of on the building. It is required where spontaneous breakage would be dangerous or expensive to replace.

Nickel sulphide (NiS) inclusions are a fraction of a millimetre in size and come from the raw glass. After tempering they are trapped in a metastable state and can expand years later, cracking the pane with no impact. Raising the glass to 290 °C ± 10 °C accelerates that transformation, so roughly 95 % of panes that would have failed on site fail in the test chamber instead.

The test is defined by EN 14179-1 (and GB 15763.4 in China), requires a certified furnace with a recorded temperature profile, and adds roughly 2–3 days to the lead time and 3–8 % to the price of the panel.

Which figures decide whether you need a heat soak test?

Holding temperature290 °C ± 10 °C
Holding time2 hours minimum
StandardEN 14179-1 / GB 15763.4
Failure rate detectedabout 95 % of NiS-critical panes
Added lead time2–3 days

What should you check on the HST report and the order?

Related: Tempered glass Jumbo glass Company fact sheet
Need a quote against your drawing?

Send the glass schedule, thickness build-up and destination port to info@cnglassworks.com or on WhatsApp (reply within 1 hour) / phone +86 138 3303 3053. A specification review and reference price come back within one working day.

Figures verified by the factory on 2026-11-02. Sizes are manufacturing limits, not project guarantees.

Price from USD ___ per sqm FOB Qinzhou, depending on thickness, coating and quantity.